Chemical Composition
| Grade Symbol |
UNS Number |
Alloy |
Elements |
Composition % |
| F316 |
S31600 |
18 chromium, 8 nickel, modified with molybdenum 316G |
Carbon |
0.08 max |
| Manganese |
2.00 max |
| Phosphorus |
0.045 max |
| Sulfur |
0.030 max |
| Silicon |
1.00 max |
| Nickel |
10.0–14.0 |
| Chromium |
16.0–18.0 |
| Molybdenum |
2.00–3.00 |
| Nitrogen |
0.10 max |
Mechanical Properties
| Property | Value |
| Tensile Strength, min, ksi [MPa] |
75 [515] |
| Yield Strength, min, ksi [MPa] |
30 [205] |
| Elongation in 2 in. [50mm] or 4D, min, % |
30 |
| Reduction or Area, min, % |
50 |
Heat Treatment
After hot working, forgings shall be cooled to a temperature below 1000 °F [538 °C] prior to heat treating in accordance with the requirements.